2-5 Solder Paste Operation Manual

Home> 2-5 Solder Paste Operation Manual

2-5 Solder Paste Operation Manual

2-5 Solder Paste Operation Manual 

2-5-1 Shelf Management


1)Store the paste between 0℃ to 10℃(4℃ to 8 ℃ is the best). It will take at least 3 hours to recover to room temperature after cold storage in the refrigerator.

2)Churn up the paste before use. 5 minutes are required in by automatic churning machine and 10min by hand.

3)Ensure that only the bottle of paste being used is open. This is intended to keep the paste fresh for future use and reduce the negative impact of the environment. Tighten the cap, both inner and outer, after use to prevent the solder paste from drying or being oxidized, therefore extending the service life of the product.

4)Use the paste according to the principle of FIFO.

5)Make sure the paste rolling continuously during printing operation. Keep the height equal to 1/2~3/4 of the scraper's. Monitor the viscosity of solder paste in the process. Smooth rolling can be conducive to transfer the paste to the underlying the stencil opening, thus a finer pattern..

6)Transfer the printed PCB to the next procedure as soon as possible (within 1 hour), to prevent solder paste from drying and viscosity degradation.

7)Don't leave the paste on PCB more than 1 hour to avoid clogging the PCB.

8)Collect the used paste with a new container to avoid old solder paste affecting the property of the new. Please refer to the corresponding requirements when dealing with used paste storage. Used paste and fresh paste mixed up in a ratio of 1:3 can be equal to the totally fresh one in property.


2-5-2 Screen Print Parameters


1) Scraper Speed: normally 10-150mm/s.

Being too fast could cause the scraper to slide or miss printing while being too slow may lead to uneven edges and taint the substrate surface.

2) Angle of the Scraper Fixation: In the range of 60°-90°, appropriate printing pressure acquired from adjustment to the angle could reach the best printing and transferring efficiency.

3) Printing Pressure: 0.1-0.3kg/c㎡.

Low pressure could lead to insufficient amount of transferring paste, and high pressure may result in undesirably thin paste layer and increase the chance of tainting the substrate surface. Please increase the pressure from the minimum gradually until it's just able to scrape off the paste from the surface of slat.

4) Hardness and Material of the Scraper: hardness 80-90 HS; material, stainless steel or rubber.


2-5-3 Cautions


1) Please read the MSDS before operation.

2) Avoid any direct contact with the solder paste by skin and clothes. If it happens, sweep off the paste with alcohol solvent immediately.

3) Avoid inhalation of steam during reflowing operation.

4) Wash hands after soldering operation and before dinner.

2-5-4 Temperature Profile Parameters:

Applied to Sn63∕Sn62-Ag2 solder pastes

 1) Preheat Zone: The highest temperature is 2.5℃/s. Excessive rising rate will cause solder-balling.

2) Soaking Zone: Keep the temperature within the range of 149-180℃/s and the temperature rising rate less than 2.5℃/s during the soaking zone, which lasts regularly from 60s to 90s.

3) Reflow Zone: The peak temperature in the reflowing zone changes in the range of 215-235℃ Make sure the temperature stays above 180℃ for 45-60S

4) Cool-Down Zone: The temperature dropping rate during cool-down zone should be kept under 4℃/s。

Note: The curve varies according to shape of the plate and function of the devices. The circumstance parameter is suggested to be 25±2℃ by temp. and 45%-65% by humidity.


2-5-5 Recommend Reflow Soldering Temperature Profile

Applied to WH-326 WH-373 solder pastes

 1) Preheat Zone: The highest temp.is 2.5℃/s in pre-heating area. Over rising rate will cause solder-balling.

2) Soak Zone:Keep the temp. within the range of 150-210℃ and the temp. rising rate under 2.5℃/s during the soaking zone. Which lasts regularly from 60s to 90s

3) Reflow Zone: The peak temp. in the reflowing zone changes in the range of 230-255℃. Temperature stays above 217℃ for 40-70S

4) Cool-Down Zone: The temperature dropping rate during cool-down zone should be kept under 4℃/s。

Note: The curve varies according to shape of the plate and function of the devices. The circumstance parameter is suggested to be 25±2℃ by temp. and 45%-65% by humidity.





Contact us

Zhongya(tianjin) Electronic Solder Technology Co.Ltd
Address:Xingfa Road,Balitai Industrial Zone,Jinnan District,Tianjin,PR China
Tel:86-022-83981122
Fax:86-022-83981133
Email:zhongyasolder@zhongyasolder.cn
中文熟妇人妻AV在线 | 国产三级在线观看 | 日韩一区二区三区多波结久久精品 | 国产成人一区二区三区 | 中文字幕在线免费观看 | 国产精品久久久久久久久久久久久 | 91拍真实国产伦偷精品 | 少妇高潮久久久久久图片 | 欧美性猛交XX乱大交 | 亚洲AV无码乱码精品国产′ | 成人精品视频99在线观看免费 | 国产精品揄拍一区二区 | 超碰视91麻豆东京热 | 亚洲无码自拍偷拍 | 四川少BBB搡BBB爽爽爽 | 国产精品久久久午夜夜伦鲁鲁 | 中文字幕无码AV在线免费 | 91在线极品盛宴 | 成人h精品动漫一区二区三区 | 国产精品一区二区内射视频 | 午夜激情视频在线观看 | 先锋影音亚洲AV每日资源网站 | 国产精品99久久久久久WWW | 国产足交在线观看 | 久久精品午夜亚洲AV无码少妇 | 蜜桃一区二区三区 | 中文字幕一区二区三区四区 | 欧美日韩国产精品自拍第1页 | 亚洲国产AⅤ精品一区二区的游戏 | 精品国产乱码久久久久久1区2区-亚洲 | 女厕精品久久久久久久 | 欧美亚洲日韩一区二区 | 昏睡迷奷无码片免费 | 成人午夜福利在线观看 | 久久精品国产亚洲AV不卡站借女 | 五十路の完熟豊満无码AV | 国产羞羞视频一区二区三区 | 福利姬这里只有精品视频在线观看 | 红桃视频成人免费视频 | 国产伦子伦对白视频 | 国产婬妇乱辈视频不卡 |