7-1 Innovative Sn-Cu Eutectic based Solder with Higer Creep Resistance


Compared with the mass of tin-based solders, Sn-Cu eutectic based solder, which contains no silver, has a superior performance-to-price ratio. It has been widely used in the domestic electronic manufacture in the processes of wave-soldering, dip soldering and manual welding.


However, low oxidation resistance of this alloy severely affected its application in high-reliability electronic products.

The main defect of this brazing filler metal is poor temperature structures, which severely affected its application in high-reliability electronic products. Low oxidation resistance is another disadvantage of this alloy, which increases the residues during the wave-soldering process and raises the cost as well.


As the problems mentioned above, we conducted thorough study. By the method of microalloy and addition of Co, Ni and P etc.,We successfully improved the properties of Sn-Cu solder, especially the high temperature stability at welding point and the oxidation resistance of brazing filler metal.


The study shows that, addition of Co and Ni can change the morphology of the compounds on the interface of solder/Copper substrate. Figure 1(a) and (b) show the significant differences in compound's morphology at the interface of the traditional Sn-Cu/Cu and SC-Co-Ni-(p)/Cu. It can be found that traces of Co and Ni have the ability to transform the coarse scalloped compound at the interface into close-grained laminar structure. Although the layer of this product could be thicker in as-welded condition, because of the dense and flat interface, stress concentration is unlikely to happen when the welding point suffers external stresses. Therefore, compared with the scalloped compound, the mechanical properties of the joint has been improved, especially the shock resistance and anti-shake performance.


Latest study shows that, this laminar compound has a prominent advantage that its high temperature stability is much better than scalloped compound's. In the high temperature aging test, its growth rate is much lower than that of scalloped compound.


More importantly, it can be found that close-grained laminar compounds effectively inhibit the formation of Cu3Sn at the side of Cu substrate. Figure 2 shows the microstructure of the interface after heating at 150℃ for 24h,t can be concluded that Cu3Sn has already generated in the scalloped compound, while there is little Cu3Sn in the close-grained laminar compound. As we all know, the fomation of Cu3Sn is due to the different diffusion velocity of Sn and Cu in the interface, as well as the appearance of Kenkidall cavity, which is the main cause of degeneration of mechanical properties, especially the Creep Resistance. At the scalloped interface, Sn and Cu diffuse easily through the scalloped Cu6Sn5, so Cu3Sn can be easily obtained; while there is no such diffusion channel in the laminar interface, so the speed of the formation of Cu3Sn is reduced greatly.


Figure 3 shows the results of creep resistance test at the joint of Sn-0.7Cu and SC-Co-Ni-P respectively after high temperature aging at 150℃ for 24h. T is observed that the creep resistant at the joint of this solder alloy is more than doubled.


At the same time, the wettability of the alloy has also been improved. Figure 4 shows the wettability test results of the two kinds of alloy on the surface of copper. The alloy is of low cost because it contains no Pb and Ag, which are either inhibited or expensive, and its welding technological performances are close to Sn-0.7Cu. It can be applied to the field of packaging of various electronic products, especially those which serve at high temperature for a long period of time.

  

Proprietary Product



Contact us

Zhongya(tianjin) Electronic Solder Technology Co.Ltd
Address:Xingfa Road,Balitai Industrial Zone,Jinnan District,Tianjin,PR China
Tel:86-022-83981122
Fax:86-022-83981133
Email:zhongyasolder@zhongyasolder.cn
3atv一区二区三区 | 一区三寸高清无码视频 | 日本在线不卡一区二区三区 | 欧美性受XXXX黑人XYX性爽 | 婷婷五月色婷婷五月天 | 久久无码精品丰满人妻 | 欧美日韩免费网站 | 中文字幕av久久爽一区 | 成人做爰黄AAA片爽爽漫画网站 | A V免费视频在线观看 | 亚洲成人综合在线 | 亚洲无码高清免费 | 91麻豆精品国产91久久综合 | 久久午夜精品无码AV片下载蘑菇 | 好爽…又高潮了毛片免费看 | 亚洲午夜在线观看 | 婷婷 cheng人 在线 | 中文字幕人妻在线 | 超碰97超碰资源总站 | 麻豆一级A片久久久乱码 | 一级毛片AAAAAA免费看对白 | 东京热无码免费A片免费下载 | 91在线观看视频 | 国产成人无码www免费视频在线观看 | 国产春色tv导航下载 | 少妇自慰喷水网站www | 少妇高潮久久久久久潘金莲 | 91制服诱惑强奸乱伦 | 国产视频一区二区在线 | 一级一级a一级a爱片免费兔兔软件 | 五月天激情国产综合婷婷婷 | 国产69久久久欧美黑人A片 | 成人无码国产精品秘 久久 EEUSS鲁丝少妇人妻片 | 亚洲午夜无码电影 | videos 国产口爆 | 国产美女裸体视频永久免费无遮挡 | 亚洲AV无码乱码精品国产蜜臀 | 男女无遮挡动图120秒免费在线观看 | 拍真实国产伦偷精品 | 天天日,天天干,天天插。 | 精品国产乱码久久久久久国产自啪 |